PAVEMENT DESIGN PRACTICAL REPORT

MODULE IV
WEIGH LOSS OF OIL AND ASPHALT (THICK FILM TEST)

GROUP I

Adam Yuta Prayoga

(1206292370)

Bimasena Heribowo Adi

(1206292351)

Christopher Kevinly

(1206223846)

Wednesson Lawijaya

(1206230593)

Date of Experiment

: 30 September 2014

Assistant

: Sinta Indrawati

Date of Approval

Signature

Score

LABORATORIUM STRUKTUR DAN MATERIAL


CIVIL ENGINEERING DEPARTMENT
FACULTY OF ENGINEERING
UNIVERSITY OF INDONESIA
DEPOK
2014

J-04 WEIGH LOSS OF OIL AND ASPHALT (THICK FILM TEST)


(PA 0304 76)
(AASHTO T 47 82)
(ASTM D 6 80)

I. PURPOSE
The purpose of this experiment is to determine weigh loss of oil and asphalt with heating and
certain thickness, the result are presented as comparison of its original weigh.

II. TOOLS
i.

Termometer

ii.

Oven that are equipped:


a. Heat adjuster until (1801)0 C.
b. Metal dish 25 cm in diameter, hangs in the oven on the vertical axis and
rotates at a speed of 5 to 6 rounds per minute.

iii.

Cup

iv.

Metal or glass cylindrical, with a flat bottom in the size: diameter 55 mm and height
35 mm.

v.

Weighing scale analytic, dengan kapasitas (0,001 200) grams.

III. SPECIMENT
a. Preparation. Mixed the sample of oil and asphalt then heated but make sure mixture
are fuly blended.
b. Pour sample about (500,5) gram inside cup after its temperature had cooled down
and weigh it with accuracy of 0.01 gram
c. Specimen need to free from water.

IV. PROCEDURE
a. Placing the test substance on the plate after the oven reaches temperature (163 1) 0
C.
b. Install thermometer on the stand that is located at a distance of 1.9 cm from the edge
of the dish with the tip of 6 mm above the dish.
c. Taking a test specimen of the oven after 5 hours to 5 hours 15 minutes.

d. Cooling the specimen at room temperature, and then weighed to the nearest 0.01 gram
(B).

V. DATA PROCESSING
CUP

WEIGH BEFORE

WEIGH AFTER

HEATING (A)

HEATING (B)

75.5gr

75.3gr

Cup + Asphalt
Cawan

37 gr

Aspal

38.5 gr

Penurunan Berat (%)

38.3 gr
0.519%

VI. ANALYSIS
a. Experiment analysis
Before the experiment is carried out, we gather ourself at the property material
laboratory to prepare our specimen. Then, we prepare all the tools that includes
thermometer, an oven, cup, cylinder and weighing scale. Firstly, we are going to mix
all the specimen by blending them till they are evenly mixed. Specimen are to be
placed at cup for about (500,5) gram and after it has been left colded weigh it for
about 0.01 gram accuracy (A). After weighing it we obtain specimen for about 38.5
gram. This specimen are used for the penetration test first before we proceed to
heating it inside the oven till 163 Co. The weigh of the specimen is about 38.3 gram
after it had been heated in the oven for more than 5 hour long.

b. Data Analysis
The result of this experiment that is obtain is the weigh the specimen after and before
it has been subjected to heating. The weigh before heating is 38.5 gram and the weigh
of the experiment after the specimen had been heated is 38.3 gram. With this result
we could also determine the percentage of weigh loss in refer to its original weigh
(

c. Error Analysis

Mixing error. Students might do some mistakes in mixing the as mixture must
be perfectly blended to avoid air void.

Estimation and Roundoff error

We did not follow the actual heating temperature and time, as we may heat the
specimen for too long.

VII. CONCLUSION

There is about 0.519% of weigh loss

VIII. REFERENCES
Fakultas Teknik Universitas Indonesia. 2009. Pedoman Praktikum Bahan
Perkerasan Jalan.