REPAIR WELDING

Removal of Defects:
The identified defect area shall be marked on the part.
The defects may be removed by grinding/thermal gouging.
Where thermal gouging is done, adopt the requirements of preheating as detailed in Heat
Treatment Manual.
However, only grinding is permitted for the last 6 mm from the root.
Removal of defects shall be verified by visual inspection, PT, MT, RT as appropriate.
The profile of ground portion shall be smooth and wide enough to permit proper fusion during
repair welding.
Repair welding shall be carried out as per the procedure for the initial weld.
Repair weld shall undergo the same type of NDE as the initial weld.
Repeat steps 2.1 to 2.6 till acceptable weld is made.
Where the defect volume is high, Cut and weld of joints is recommended.
Where a specific repair procedure is supplied by the Manufacturing Unit, the same shall be
followed.
RECORDS :
Records pertaining to the repairs like Welder, NDE records shall be maintained.
SAFE PRACTICES IN WELDING
All combustible materials should be removed or safely protected within a radius of 35 ft. (11m)
around the work area.

PRE - ASSEMBLY AND WELDING OF CEILING GIRDERS


PRE-ASSEMBLY FIT UP & ALIGNMENT:
Do pre-assembly fit up and alignment of girder pieces following shop match marks. Use
L clamps and wedges (Tack welds are not permitted on the weld joints ) for web
alignment to keep the joint free during welding of flange joints to facilitate weld
shrinkage.
Check, measure and record the following for the pre-assembly before welding (Sketch2A/ Sketch 2B) (Also to measure & record after welding & PWHT)
-

Sweep by piano wire on bottom flange (max 3mm at joints & 10mm for assy)
Camber by water level on bottom flange (max 3mm at joint & 10mm for assy)
Length between girder pin bolt hole centers (overall max 15 mm)

Diagonal difference (max 15 mm)


Root gap (Flange=4 to 6mm; Web=6 to 8mm)
Web verticality by plumb (To monitor distortion before & after welding)
Distance between punch marks at weld joints (To monitor weld shrinkage)

NOTE:
Flange root gap will be absorbed during welding as weld shrinkage.
Tolerances given above are indicative.
To accommodate weld shrinkage, ensure web root gap 3-4 mm more than flange root gap
Length before welding = Drg length + root gap of flange joints
Ensure temporary locking & welding of the pre-assembly before start of girder welding
(Sketch-3) with provision for longitudinal movement during welding to avoid
accumulation of thermal stresses & facilitates controlled weld shrinkage
NON-DESTRUCTIVE EXAMINATION (NDE):
FLANGE BUTT JOINT:
Root Back grinding: 100% LPI Intermediate radiography for thickness > 80mm (desired)
On completion of weld
100 % RT for thickness >32mm & < 80mm
100 % UT for thickness > 80mm
100 % MPI for thickness > 25mm (after PWHT)
WEB BUTT JOINT:
Root Back grinding: 100% LPI
On completion of weld
Spot RT for thickness <32mm 100% RT for thickness >32mm
FILLET WELDS:
Between flange and web:100% MPI (after PWHT)

PRE-HEATING, POST HEATING & PWHT REQUIREMENTS:


PWHT CYCLE:
Weld thermocouples on top & bottom flange and web joints (as per sketch-4). Arrange
PWHT of flange and web joints with electric resistance coil heaters. Issue PWHT job
card. (Refer Exhibit) Select midpoint of temperature range and control cycle within a
tolerance of 15C. Record PWHT cycle with a calibrated temperature recorder
Identify PWHT chart with chart No & date and PWHT cycle with weld joint number.
Review the cycle and record observations / acceptance on chart .

FINAL INSPECTION (AFTER PWHT):

Grind / buff the Flange Butt & Fillet joints (site welds) and conduct MPI.

Clean all Site welds and paint with two coats of red oxide primer.
Repeat all checks under section B and record measurements (Sketch 2A / 2B).
Punch centre line of girder on flange thicknesses and top surface of top flange
OTHER PREPARATORY WORKS FOR ERECTION:
Blue match girder pin bottom piece with column and complete support lugs welding in
position. Subsequently blue match girder pin top piece with girder, tack weld support
lugs in position, remove and complete lugs welding. Conduct LPI & maintain record.

Open the girder pin assembly, buff clean the pin and seating surfaces, apply grease, reassemble and lock the pin with pin assembly by tack welding of lock plates.
Mount the girder pin assembly on ceiling girder for easiness of erection of girder
pins. Buff Clean Cement wash in the HSFG bolt area and cleat angles at WBs
location

WELDING SEQUENCE FOR CEILING GIRDER


Sl.
No.

SEQ.
No.

Pre heat and weld root run at flange

Weld root run at flange

WELDING SEQUENCE

Repeat step 1 and 2 and weld three runs


Post heat and cool to room temperature

4
5

Back grind and do LPI (at flange)


3

Pre heat and weld Root + Three runs (at other side of the flange)

Follow steps 1, 2 and 3 alternatively and welding upto 60% of the thickness of the

Correct the mismatch and check the root gap of the web and grind if required

Weld root run (at web)

Weld root run (at web)

10

Weld two run (at web)

11

Weld two run (at web), post heat and cool to room temperature

12

Back grinding and do LP (at web)

13

Grind the flange welding and take intermediate RT if required

14

Root run (at other side of the web)

15

Root run (at other side of the web)

16

Weld two run at web

17

Weld two run at web

18

1,2

Weld three run at flange

19

Weld three run at flange

20
21
22

4
5

Follow steps 1,2 and 3 alternatively and complete the flange welding
Weld three run at web
Weld three run at web

23

Weld three run at web

24
25
26

7
8

Weld three run at web


Follow steps 4, 5,6,7 alternatively and complete the web welding
Weld root +two run (at flange +web) - Fillet weld

27

Weld root +two run (at flange +web) - Fillet weld

28

Follow step 8 and 9 alternatively(each three run and complete flange +web fillet
welding)

ERECTION WELDING PRACTICE FOR SA335 P91 MATERIAL


Color Code: Brown & Red
Hard Stamping: Specification, Heat No, Size.
Paint / Stencil: WO DU, as per the relevant drg & document.
When any defect like crack, lamination, and deposit noticed during visual examination the same shall
be confirmed by Liquid Penetrant Inspection. If confirmed, it shall be referred to unit.
The fit-up shall be as per drawing. Root gap shall be 2 to 4 mm; root mismatch
shall be within 1-mm. Suitable Reference punch marks shall be made on both the pipes (at least
on three axis).
At 200 mm from the EP for UT.
At 1000 mm from the EP for identifying weld during PWHT.
No Preheating is required for fixing T / C with resistance spot welding
Following are the equipment / facilities for heating cycles.
Heating methods: Induction heating
Thermocouples: Ni-Cr / Ni-Al of 0.5 mm gauge size.
Temp.Recorders : 6 Points / 12 Points.
ARRANGEMENT FOR PURGING:
Argon gas of 99.99% conforming to Gr 2 IS 5760 1998 shall be used for purging the root side
of weld.
The flow rate is to be maintained during purging is 10 to 26 litres/minute and for shielding during GTAW
is 8 to14 litres/minute.(A minimum flow rate as per welding Procedure specification shall be
maintained).
Start purging from inside of pipe when root temperature reaches 220deg C. Provide continuous and
adequate Argon Gas to ensure complete purging in the root area.
The minimum pre-flushing time for purging before start of welding shall be 5 minutes,
irrespective of the pipe size.
Wherever possible, solid purging gas chambers are to be used which can be removed after welding. If
not possible, only water-soluble paper is to be used. Plastic foils that are water- soluble are NOT
acceptable.
USING ALUMINIUM DAM ARRANGEMENT:
The Aluminum discs shall be firmly secured with a thin wire rope. After completion of the root
welding followed by two filler passes, the disc may be pulled outwards softly.

CAUTION : ENSURE REMOVAL OF PURGE DAM ARRANGEMENT AFTER WELDING

USING OF WATER SOLUBLE PAPER:


The dams can be made of water-soluble paper for creating the purging
chamber. The advantage in such dam arrangement is that dissolving in water
can flush the dams. The following are different methods used.

WELDING / WELDERS QUALIFICATION:


The drying Temp shall be 200 - 300 deg C for two hours if it is not specified by the manufacturer.
Portable flasks shall be used by the welders for carrying electrodes to the place of use. The electrodes
shall be kept at minimum100 deg C in the flask. Welding shall be carried out with short arc and stringer
bead technique only.
The inter-pass temperature shall not exceed 350 deg C. After completion of Welding bring down the
temp to 80 - 100 deg C and hold it at this temp for one hour minimum. The PWHT shall commence
after completing one hour of soaking.
CAUTION: - No LPI / Wet MPI shall be carried out on weld before PWHT.

POST WELD HEAT TREATMENT:


Arrangements: - A minimum of four thermocouples shall be placed such that at least two are on the
weld and the other two on the base material on either side of the weld within the heating band at 180
degrees apart about 50mm from the weld joint. Two stand by thermocouple shall also be provided on
the weld in case of any failure of the thermocouple
The PWHT temp for P91 with P91 material shall be 760 + 10 deg C and the soaking time
Shall be 2.5 minutes per mm of weld thickness, subject to a MINIMUM OF TWO HOURS. All records
shall be reviewed by Welding Engineer prior to PWHT clearance. Heating shall be done by Induction
heating only.
The rate of heating / cooling :- Thickness
(above 350 deg C)
Thickness
Thickness
Thickness = Actual thickness as measured.

up to 50mm - 110 deg C / hr.(max)


50 to 75mm - 75 deg C / hr.(max)
above 75mm - 55 deg C / hr.(max)

INSULATION: The width of the insulation band beyond the heating band shall be at least two times
the heating band width on either side of the weldment.
PREVENTIVE MEASURES DURING POWER FAILURE AND NON-FUNCTIONING OF
EQUIPMENT'S:
During start of preheating:
In case of any power failure/interruption during preheating, the weld fit-up shall be insulated and brought
to room temperature. After the electric supply resumes the joint shall be preheated
During GTAW / SMAW:
Use gas burner arrangement to maintain the temperature at 80 deg - 100 deg C up to a length of 50mm
on either side from weld centerline along the complete circumference of the pipe. Root welding shall
be continued after power is restored and preheating temperature is raised to 220 deg C. During the
above period temperature shall be recorded through contact type Thermometer.

During cooling cycle after SMAW welding to holding temperature at 80 to 100 deg C for one hour.
Care shall be taken to avoid faster cooling rate by adequate insulation. The required temp 8 0
- 100 deg C shall be maintained by gas burner arrangements till power resumes / start o f PWHT.

Power Failure during cooling / holding

Temp
in deg c

Theoretical curve
Actual curve

350
220
100
80

RT

During power

cut
Time

Fig - 5

After power resumes


Maintain 80 - 100 C for a min period
One hour by immediate insulation and
heating by gas

During post weld heat treatment; the following shall be followed:


During heating cycle, the whole operation to be repeated from the beginning.

2) During soaking
Heat treat (soak) subsequently for the entire duration. (Complete period).
Temp
in deg c

T
T1

760 10
Actual curve

350

Power cut
Theoretical curve

220

T1 =T

100
80
RT
Time

3) During cooling (above 350 deg C).


Reheat to soaking temperature and cool at the required rate.
Temp should not be allowed to fall below 80 100 deg C. Gas burner arrangement shall be used to
maintain the temperature.

In all the above cases (a to d) the temp. Measurement on the weld joint by means of contact type
calibrated temp. Gauges shall be employed to record the temperature at regular Intervals of 15
minutes in the log book by Quality Assurance Engineer /Welding Engineer.
TEMPERATURE MONITORING:
The welding and heat treatment chart given in Figure 9 shall be followed for the following details.
The actual PWHT chart shall be monitored for the following:
Preheat
Inter pass Temperature (GTAW + SMAW)
Controlled cooling and Holding at 80-100 Deg C for minimum one hour under insulation. Start
PWHT after minimum one hour of soaking.
Heating to PWHT
Soaking at PWHT
Cooling to 350 Deg C
Cooling to Room Temperature (under insulation)
CAUTION:

THE PWHT TEMP. SHALL NOT DEVIATE FROM THE VALUES SPECIFIED IN THE CHART
RANGE SINCE ANY DEVIATIONS TO THE SPECIFIED HOLDING TEMPERATURE RANGE,
WILL ADVERSLY AFFECT THE MECHANICAL PROPERTIES OF THE WELDMENT AND
MAY LEAD TO REJECTION OF THE WELDMENT. THE WELD JOINTS SHOULD BE KEPT
DRY.UNDER NO CIRCUMSTANCES ANY WATER/LIQUID IS ALLOWED TO COME IN
CONTACT WITH WELD AS WELL AS PREHEATED PORTION OF PIPE.

NONDESTRUCTIVE EXAMINATION:
The calibration blocks used shall be of same material specification (P91) dia & thickness.
The UT equipment shall be calibrated prior to use and should be of digital type Krautkramer Model
USN 50 or equivalent or higher version, capable of storing calibration data as well as ultrasonic test
results as per UT-21
All record able indications will be stored in memory of either the digital flaw detector or a
PC for review at a later period.
HARDNESS SURVEY:

The max allowable hardness at weld and parent metal shall be 300 HV10. Joints having
hardness above 300 HV shall be reheat treated and hardness shall be checked again. If
hardness is still more refer to unit.
PM 1
WELD
PM 2

270

90

180
Figure 10
LOCATION
READINGS
0
90
180
270

AVE

PM: PARENT MATERIAL

WELD
2

AVE

AVE

AVE: AVERAGE

COMBINATION WELDING:
SOAKING TIME FOR COMBINATION WELDING:
WPS N0. Material Temp.,
1035
P91+P22 745 15 C
MS W0454. P91+X22 750 10 C

Soaking time
2.5mts / mm minimum one hour
2.5mts / mm minimum two hour for thickness upto
50 mm and minimum four hours for thickness
above 50 mm.
However the precautions as required for P91shall be fully taken care of.

DOs and DONTs during P 91 welding, heat treatment and NDE at construction site:
DOS:
a) Cutting by Band saw/Hack saw/Machining.
b) Pipes Edge Preparation by machining. Machining shall be done without excessive pressure to
prevent heating up of pipe
c) Grinding may be done on exceptional cases after approval and taking adequate care to prevent
overheating.
d) Thermocouple wire (hot/Cold junctions) shall be welded with condenser discharge portable
spot-welding equipment.
e) Reserve Thermocouples shall be made available, in case of failure of connected thermocouple
elements.
f) Ensure adequate Argon Gas for complete purging of air inside the pipe before starting GTAW
root welding.
g) Ensure Preheating at 220 Deg.C minimum before GTAW root welding.
h) Start preheating only after clearance from Welding engineer / Quality assurance engineer for
weld fit-up and alignment of the joint as well as fixing of Thermocouple connections ( for
Induction heating)
i) Do visual inspection on root weld maintaining weld preheating temp.
j) Continue Argon purging until the GTAW root welding followed by minimum two
fille
r passes of SMAW, is completed.
k) Perform partial root welding to facilitate fit-up if necessary.
l) Ensure that only one layer of root welding using TGS 2CM filler wire (2 Cr 1 Mo) is
deposited. (Wherever specified).
m) Ensure proper use of TIG wires as identified by color coding or suitable hard punching.
n) Keep the GTAW wires in absolutely clean condition and free from oil, rust, etc.
o) Dry the SMAW electrodes before use.
p) Ensure the interpass temperature is less than 350 Deg.C.
q) Hold at 80-100 Deg.C for a period of Minimum 1 hour before the start of PWHT.
r)

Record entire heating cycle on Chart through recorders.

s) Exercise control during grinding of weld and adjoining base metal while removing
surface/sub-surface defects or during preparation for NDE.
t) Ensure no contact with moisture during preheat, welding, post heat and PWHT of
Weld Joints.
u) Ensure removal of argon purging arrangements after welding.
v) Use short Arc o n l y . The maximum weaving shall be limited to 1.5 times the dia of
the electrode.

DONTs:
a) Avoid Oxy-Acetylene flame cutting.
b) Avoid Weld-build up to correct the weld end-d1 or to set right the lip of the weld bevel.
c) Avoid Arc strike on materials at the time of weld fit up or during welding.
d) Do not Tack weld the Thermocouple wires with Manual Arc/TIG welding?
e) NO GTAW root welding without thorough purging of root area.
f) Do not use Oxy-acetylene flame heating for any heating requirements.
g) Do not use Thermal chalks on the weld groove.
h) Do not stop argon purging till completion of GTAW root welding and two layers of SMAW.
i) No Tack welding or Bridge piece welding is permitted.
j) Do not use unidentified TIG wires or electrodes.
k) Do not exceed the maximum interpass temperature indicated in WPS
l) Do not allow moisture, rain, water, cold wind, cold draft etc. to come in contact with the weld
zone or heating zone during the entire cycle from preheat to PWHT.
m) Do not exceed the limits of PWHT soaking temperature.
n) Do not Interrupt the Welding/heating cycle except for unavoidable power failures
o)
Do not use uncalibrated equipment for temperature measurement during heating, welding,
post weld, heat treating etc.,
WHAT IS ARGON?
Argon is chemically-inert, monatomic gas, heavy and available in quantity at reasonable cost. Its
chemical symbol is Ar. Atomic weight is 40. Molecular weight is 40.
The compressed argon is supplied in cylinders and liquid argon is supplied in tanks. The cylinder used
for argon will have the body colour of BLUE without band, size of 25 cms dia. & 1.5 m length,
capacity of 6.2 M3 and pressure when fully charged at 150C (approx) 137 Kg/Cm2 (1949 psi).
PURITY LEVEL OF ARGON
INDIAN STANDARD for ARGON, Compressed & Liquid Specification no. IS 5760: 1998 shall be
referred.
There are 3 grades of argon, namely:
Grade 1 : Ultra high purity argon for use in electronics and allied industries and indirect reading vacuum
spectrograph,
Grade 2 : High purity argon for use in lamp and allied industries and
Grade 3 : Commercial grade argon for use in welding industry and for other metallurgical operations.

Accordingly the argon shall comply with the requirements given below:
Sl.
No. CHARACTERISTIC
i.
Oxygen, ppm, Max.
ii.
Nitrogen, ppm, Max.
iii. Hydrogen, ppm, Max.
iv. Water vapours, ppm. Max.
v.
Carbon dioxide, ppm, Max.
vi. Carbon monoxide, ppm, Max.
vii. Hydrocarbons, ppm, Max.

REQUIREMENT
Grade 1 Grade 2 Grade 3
0.5
5.0
10.0
2.0
10.0
300
1.0
2.0
5.0
0.5
4.0
7.0
0.5
0.5
3.0
0.5
0.5
2.0
0.2
0.5
-

PURCHASE SPECIFICATION FOR ARGON:


Argon as per Grade 3 of IS-5760: 1998 Rev 02 with Oxygen & Water Vapours restricted to max. 7
PPM each and with Argon purity level of min. 99.99%. The supply should accompany Test Certificate
for the batch indicating individual element PPM level and overall purity level.

GENERAL TOLERANCES FOR WELDED STRUCTURES - (FORM AND POSITION)


GENERAL:
Tolerance on form and position as defined in this standard are permissible variations from the
geometrically ideal form and position corresponding to the accuracies commonly obtained in workshops.
The standard covers tolerances on straightness, flatness and parallelism.
This standard is based on DIN 8570 Part 3 - 1987General tolerances for machined components are
covered in corporate standard AA 023 02 08.
Refer Corporate Standard AA 062 11 04 for general tolerances for lengths and angles of welded
components, assemblies and structures.
TOLERANCES ON STRAIGHTNESS, FLATNESS AND PARALLELISM
Nominal Dimension Range (larger side length of surface) - mm
Grade
Above Above Above Above Above Above
Above Above Above
of accu1000
2000 4000
8000 12000 16000 Above
30 to 120 to 315 to
racy
to
to
to
to
to
to
20000
120
315
1000
2000
4000 8000 12000 16000 20000
E
0.5
1
1.5
2
3
4
5
6
7
8
F
1
1.5
3
4.5
6
8
10
12
14
16
G
1.5
3
5.5
9
11
16
20
22
25
25
H
2.5
5
9
14
18
26
32
36
40
40

TESTING:
STRAIGHTNESS:
The edge of the welded component and the straight edge can be arranged in relation to each other so that
the end points of the measured length are the same distance apart from the ends of the straight edge. The
distances between the edge and the straight edge should be measured.
FLATNESS:
A measuring plane can be set up outside the welded component parallel to the limiting planes at any desired
distance. For example this can be done with optical instruments, flexible tube liquid levels, tension wires,
clamp plates, surface plates and machine beds.
PARALLELISM:
Any of the measuring devices mentioned above can be used to set up a measuring plane outside the welded
component parallel to its reference plane.The distance from the actual surface to the measuring plane is
measured.
The position of the reference surface (= surface after machining) is dimensionally determined.
Dimension a1 gives the required finished height of the foundation. Dimension a2 gives the minimum
thickness of the support.
The distance between the reference plane and the measuring plane is greater than: hmax by the minimum
possible thickness of the machining allowance b. The variation of the actual surface (=surface before
machining) from the reference plane must be within the tolerance on parallelism. Maximum variation is
hmax - hmin
t
Note: The tolerance on form and position as per this standard may be mentioned on the drawing in addition
to the linear tolerances as per AA 062 11 04 wherever required.

REPAIR PROCEDURE FOR GREY CAST IRON CASTINGS


IS 210 Gr. 20 & Gr.25
ELECTRODES:
Low heat nickel iron electrodes (ENi CI and ENiFe-CI type) should be used. The following
brands are recommended for repairs:
ENi CI : 1) NFM (D&H Secheron) 2) CASTRON KALT ( Modi) 3) FERROLOID -4 (ESAB)
ENiFe-CI : 1) ESAB 802 2) 1111CI (D&H Secheron)

WELDING PROCEDURE:
To ensure maximum freedom from porosity in weld deposits, nickel iron electrodes should be re-baked
for at least one hour at 260C in a well ventilated electric oven and either used immediately or stored in
a similar oven at 120C until used.
The welding current should be kept as slow as possible consistent with smooth operation and a good
wash at the sides of the joint.
Wherever possible the casting should be positioned for down hand welding operation. When extra-long
welds or several repair positions are involved it is preferable to stagger the welding operation to distribute
the heat and to minimize the distortion.
Manipulation of the electrode:
It is preferable to use stringer bead technique, with beads not > 50 to 75 mm in length, slight weaving of
the electrode may be done to obtain better wash, but in no case the width of the deposit should be > 3
times the nominal dia. of the electrode.
PREHEATING:
Preheating is normally not required. Where preheating is resorted to, the entire casting should be
preheated. Interpass temperature should not exceed 250C.
Peening of the weldment after the weld cools down may be done to reduce the shrinkage
stresses.
INSPECTION:
In addition to visual examination, non-destructive tests like liquid penetrant inspection might be
employed on repaired areas to ensure freedom from cracks.

SPECIAL INSTRUCTIONS FOR THE REPAIR OF STEAM TURBINE

Material specification

: GS-C25, 422710, 422643, SA 216


WCB

Removal of defects

: Defects shall be removed by grinding /


machining.

Inspection of pre-welding

: Complete elimination of defects shall


be

ensured

by

LPI

MPI

Radiography.
4

Welding procedure :
a) Welder

: Qualified as per ASME Sec.IX / IBR

b) Process

: SMAW

c) Electrode

: E7018-A1. Properly baked electrodes


to be used.

d) Position

: The welding shall be done in the flat


position as far as possible.

e) Arc current

: 2.50 mm (60-80 amps)


3.15 mm (90-130 amps)
4.00 mm (140-180 amps)
5.00 mm (190-240 amps)

f) Preheating

: Up to 30 mm thickness } 10C
30-100 mm thickness } 100C
101-200 mm thickness } 150C

g) Inter pass temperature

: 350C max.

Stress relief

: Below 40 mm thickness no stress


relief is required.
Above 40-200 mm thickness stress
relieve at 600-620C for 3 hours.

Inspection of Post welding

: MPI followed by UT.

REPAIR WELDING PROCEDURE


1

Material specification

: GS-17CrMoV511, 21CrMoV57V,
21CrMoV57, 422731.1, 422743.1,
422744.1, 422745.1

Removal of defects

: Defects shall be removed by grinding


or machining and ensure complete
removal by LPI / MPI.

Welding procedure :
a) Welder

: Qualified as per ASME Sec.IX / IBR

b) Process

: SMAW

c) Electrode

: E9018B3. Properly baked electrodes to


be used.

d) Arc current

: 2.50 mm (60-80 amps)


3.15 mm (90-130 amps)
4.00 mm (140-180 amps)
5.00 mm (190-240 amps)

e) Preheating

: 300C, continue this temp. Throughout


the welding operation.

f) Inter pass temperature

: 375C max.

Post weld heat treatment

: The casing has to be stress elieved as


per code of practice in welding
procedure specification.

Inspection after Post weld heat treatment

: MPI followed by UT.

REPAIR WELDING PROCEDURE


1

Material specification

: GS-17CrMo55(P4), A182F12,
A217WC6, A387-12

Removal of defects

: Defects shall be removed by grinding


or machining and ensure complete
removal by LPI.

Welding procedure :
a) Welder

: Qualified as per ASME Sec.IX

b) Electrode

: E8018B2. Properly baked electrodes


to be used.

d) Arc current

: 4.00 mm (140-180 amps)


5.00 mm (190-240 amps)

e) Preheating

: 250C, maintain this temp. throughout


the welding operation.

f) Inter pass temperature

: 350C max.

Post weld heat treatment

: Maintain the temp. at 300C for about


2-3 hours and allow it to cool under
asbestos.

Inspection after Post weld heat treatment

: MPI followed by UT.

Note: If weld repair is extensive, i.e. thickness of weld metal is more than 10 mm,
the casing has to be stress relieved as per the code of practice.

GENERAL
In GMAW the consumable is a wire spool, which is continuously fed by a motor. This
consumable as well as the shielding gas come out through a hand held torch and the torch is
moved manually.
The method has two commonly used variants:
(a)Metal Inert Gas (MIG) welding (an example is the welding of aluminum bus ducts at site)
(b)Metal Active Gas (MAG) welding (an example is steel chimney fabrication at site)
While Argon is almost always used in MIG welding for shielding the arc, Carbon Dioxide or
Carbon Dioxide with Argon is used for MAG welding.
ADVANTAGES OF GMAW
The advantages of GMAW over SMAW are:
(a)
High welding speed due to continuous feed of filler metal and high deposition rate
(b)
No slag removal and no slag inclusion
(c)
Higher deposition efficiency
(d)
Higher arcing time
(e)
Low hydrogen content in weld metal
VARIABLES AFFECTING WELD QUALITY
The variables which affect weld quality in GMAW ARE:
(a)
Welding current
(b)
Polarity
(c)
Arc Voltage
(d)
Travel speed
(e)
Electrode extension
(f)
Weld joint position
(g)
Electrode diameter
(h)
Shielding gas composition
(i)
Gas flow rate
Current range :
120 to 160 Amps
Voltage range :
19 to 22 Volts
Electrode consumed (cm / M) :
3 to 3.8 M / Min.
Current AC or DC
:
DC
Polarity
:
EP
Size of reinforcement :
1.5 to 2 mm
Whether removed
:
No
Inspection and test schedules :
As per IS 7307 PT-1

WELDING PROCEDURE DATA SHEET


Welding Process

: Semi-Auto

Material specification

: IS 2062 Gr.A

Thickness
Plate
Pipe diameter

: 8 mm
: --

Filler metal specification

: IS-6419 84-C504 (ER-7086)

Weld metal analysis

: NA
FLUX OR SHIELDING GAS

Flux trade Name or composition

: NA

Shielding gas composition

: 99.7% CO2

Trade Name

: NA

Flow rate

: 10-15 LPM

Backing strip used

: NA

Pre-heat temperature range

: 10 C Min.

Interpass temperature range

: 265 C Max.

Post Weld Heat Treatment

: NA

WELDING PROCEDURE
Single or Multi-pass

: Multi-pass

Single or Multiple Arc

: Single

Welding position(s)

: Horizontal Vertical
FOR INFORMATION ONLY

Electrode and filler wire diameter

: 1.2 mm

Trade Name

: CTTOFIL(ADVANI)

Type of backing

: NA

Fore hand and back hand

: NA

WHAT IS ORBITAL WELDING


Definition
The term Orbital-Welding is based on the Latin word ORBIS = circle. This has been adopted
primarily by aerospace and used in terms of Orbit (n.) or Orbital (adj.) for the trajectory of a
man- made or natural satellite or around a celestial body.
The combination Orbital and Welding specifies a process by which an arc travels
circumferentially around a work piece (usually a tube or pipe).
The concept Orbital Welding is basically a loosely defined term that is usually used for
process only, where the arc travels at least 360 degrees around the work piece without
interruption.
Consequently, processes, which interrupt the full 360-weld sequence such as for better
puddle control (often used for MIG/MAG welding, using the down-hand welding sequence
in 2 half- circles), cannot truly be called orbital welding.
INSTRUCTIONS FOR CARRYING OUT CONDENSER PLATE AND NECK WELDING:
The welding of the condenser is performed by step back seam method i.e. from tack weld to
tack weld. Subsequent filling welds after tack welding are always performed in the opposite
direction.