Beruflich Dokumente
Kultur Dokumente
Micro-structural characterization
Optical Microscopy
Evaluation of Mechanical
Fig 5.1(a)Aluminium Can Ac Fig 5.1(b)Aluminium Can+4% RHA
Properties
Tensile Test(UTS,YTS)
Hardness Test
Tensile Test Results:-
Table :5.2UTS values of Al Can and its RHA composites
SL Alloy composite UTS % Increased in strength
NO Designation
Hardness Test Result:
1 Al Can 219.2 -
Table :5.1 Hardness of Aluminium can and its composites
2 Al Can + 4% RHA 230.9 5.37
SL Alloy/Composite BHN(Hardness) % increase in
3 Al Can + 8% RHA 252.8 15.32
NO Designation Hardness
4 Al Can + 12% RHA 271.5 23.85
1 Al can 5 83 6.95
10 86 7.20
15 173 14.4
2 Al + 4% 5 61 5.10
10 77 6.45
Fig :5.4Percentage elongation values of Al Can and its RHA
15 83 6.95
composites
3 Al + 8% 5 47 3.93
From Fig 5.4 Aluminium can has the highest %
10 48 4.02
Elongation and has the value of % and RHA increased
the ductility decreased from the table 15 52 4.35