Weld Face

A B
Measure from this datum only

Undercut L=1.0 Incomplete filled


D=0.5 groove + lack of
20 40 Incomplete filled Slag inclusion L=23 215
140 side wall fusion
groove L=20 L=41

Undercut D=1.5 L=43 Sharp Incomplete filled


125 253
groove + lack of side
wall fusion L=50 Crater pipe
L=1

Hard stamping 162


L=43 Arc strike
85 L=43

Mechanical damage noted throughout parent plate, all dimensions in mm.

Notes:

Excess Weld Metal = 4mm Linear Misalignment = 2.5mm Toe Blend = Poor Weld width = 16mm
WIS 5 Plate Training Sample 1. Issue1. Date 02-10
Visual Inspection Plate Report Sample Training 1.

Weld Root

A Measure from this datum only B

Me
asu Excessive root
width + Poor stop/start + Lack of root
re 20 120 173
Concave root penetration W=9 crater pipe L=5 227 fusion + poor
fro L=50 L=20 H=3.5 stop/start L=5
m
this
dat 8 Crater Crater pipe
234
um pipe L=7 L=3
onl 200
y

Tack weld
L=32

Mechanical damage noted throughout parent plate, all dimensions in mm.

Notes:

Penetration Height = 4mm Toe Blend = Poor Weld width = 9mm Misalignment = 3mm Angular distortion = 2mm