Thermanit 25/14 EW 309L-17

Rutile covered electrode

Classifications EN 1600 AWS A 5.4 Mat. No.


E 23 12 L R 1 2 E309L-17 1.4332

Characteristics Well suited for fabricating austenitic/ferritic joints at max. Welding instruction
and field of use application temperature 300 °C (572 °F). Stainless, wet corro- Materials Preheating Postweld heat treatment
sion up to 350 °C (662 °F). Suitable for depositing intermediate
Joining CrNi(Mo,N) According to ferritic No postweld heat treatment above
layers when welding clad products. For joining unalloyed/
austenitic steels to un- parent metal; 300 °C (572 °F) – risk of carbide
low alloy steels/cast steel grades or stainless/heat resistant
alloyed/low alloy steels/ mostly not necessary precipitation in the weld fusion zone,
Cr steels/cast steel grades to austenitic steels/cast steel grades.
cast steel grades loss of toughness, risk of fracturing
For depositing intermediate layers when welding the clad side
of plates of low carbon, unstabilized or stabilized CrNi(Mo,N)
Joining CrNi(Mo,N) According to ferritic According to the parent metals.
austenitic metals.
austenitic to stainless/ parent metal Attention must be paid to resistance
heat resistant Cr steels/ to intercrystalline corrosion and to
Materials TÜV certified parent metals cast steel grades susceptibility of the austenitic metal
X10CrNiMoNb18-12 (1.4583) combined with ferritic steels up to side to embrittlement
fine grained structural steel S355N. Weld cladding (1st Layer)
on ferritic steels up to S355N and 20MnMoNi45; Cladded plates and According to ferritic Attention must be paid to resistance
Joints: of and between high-tensile, unalloyed and alloyed quen- parent metals with parent metal to intercrystalline corrosion and to
ched and temered steels, stainless, ferritic Cr and austenitic austenitic CrNi(Mo,N) susceptibility of the austenitic metal
CrNi steels, high manganese steels. cladding side to embrittlement
Weld claddings: for first layer of chemical resistant claddings on
ferritic-pearlitic steels up to fine grained steel S500N used in
steam boiler and pressure boiler construction, moreover for
creep resistant fine grained structural steels 22NiMoCr4-7 acc. Welding position Polarity = + / ~
to leaflet “SEW-Werkstoffblatt” No. 365, 366, 20MnMoNi5-5 and
G18NiMoCr3-7.

Typical analysis C Si Mn Cr Ni
in % <0.04 <0.9 0.8 24.5 13.0 Approvals TÜV (Certificate No. 0424) Controlas (0287)
CWB
Mechanical proper- Heat- Yield strength Yield strength Tensile Elongation Impact values
ties of the weld treatment 0.2% 1.0% strength (L0=5d0) in J CVN
metal according N/mm2 N/mm2 N/mm2 %
Packaging, weights Dimensions (mm) pcs./pack kg/pack Amperage A
to EN 1597-1 AW 400 430 550 30 55 and amperages 2.5 x 350 220 4.7 50- 80
(min. values at RT)
3.2 x 350 130 4.4 60-110
4.0 x 350 90 4.6 90-150
Structure Austenite with part ferrite 5.0 x 450 60 6.1 150-210

140 Böhler Schweisstechnik Deutschland GmbH – 09_2005 Böhler Schweisstechnik Deutschland GmbH – 09_2005 141