Sie sind auf Seite 1von 1

Thermanit 17/06

Basic covered electrode

Classifications EN 1600 Mat. No.


E Z17 6 B 2 2 앒1.4405

Welding instruction
Characteristics Stainless. Corrosion resistant similar to matching steels/cast
and field of use steel grades. Higher resistance to corrosion and corrosion Materials Preheating Postweld heat treatment
fatigue cracking than Thermanit 13/04. Matching/similar Up to 10 mm wall thickness: Tempering or quenching
Joining and surfacing on matching 13 - 17 % Cr/Ni(Mo) steels/cast steel 100-150 °C (212-302 °F). and tempering according
steels/cast steel grades. grades Over 10 mm wall thickness: to parent metal
150-200 °C (302-392 °F)

Materials (G)X5CrNiMo16-5 (1.4405); X4CrNiMo16-5 (1.4418)


matching/similar soft martensitic forging and cast steels

Typical analysis C Si Mn Cr Mo Ni
in % Welding position Polarity = +
<0.04 0.3 0.5 17.0 1.0 5.5

Mechanical proper- Heat- Yield strength Tensile Elongation Impact values


ties of the weld treatment 0.2 % strength (L0=5d0) in J
metal according N/mm2 N/mm2 % CVN
to EN 1597-1 620°C / 4 h: 570 800 15 40
(min. values at RT)

Packaging, weights Dimensions (mm) pcs./pack kg/pack Amperage A


and amperages 3.2 x 350 160 5.0 70-110
Structure Martensite, suitable for quenching and tempering 4.0 x 350 110 5.0 90-140

118 Böhler Schweisstechnik Deutschland GmbH – 09_2005 Böhler Schweisstechnik Deutschland GmbH – 09_2005 119