General information
Classification High alumina product type HA85 ISO 10081-1
Main raw material components Sintered alumina
Bonding type Ceramic
Main Application(s) Chem/petroch/oth.EEC

Environmental indicators
Product Carbon Footprint 2,253 [t CO2e/t prod.] ISO 14067
The Carbon Footprint of the Product (CFP) has been calculated following the principles of ISO 14067.

Chemical analysis
Al2O3 Fe2O3 SiO2 TiO2 Na2O

91,5% 0,2% 7,8% 0,1% 0,1%


Determination on fired substance (1025 °C / 1877 °F) acc. to ISO 12677

Physical properties
Bulk Density 2,96 [g/cm3] ISO 5017
Apparent Porosity 17,2 [vol%] ISO 5017
Cold Crushing Strength 110,0 [N/mm2] ISO 10059-1

The indicated values are standard values, i.e. values taken over a longer representative period of time according to either valid test
standards or internal test methods. They may not be regarded as committed specifications and therefore not as guaranteed
properties. We reserve the right to further technical developments and new editions of technical product information.

Revision: 01. MAY. 2022

RESISTAL A90-MX 1 / 2
Technical data sheet

RESISTAL A90-MX
Modulus of Rupture 10,0 [N/mm2] ISO 5014
2
Hot Modulus of Rupt. (1400 °C / 2552 °F) 4,2 [N/mm ] ISO 5013
Thermal Expansion 1000 °C / 1832 °F 0,70 [%] EN 993-19
1400 °C / 2552 °F 1,00 [%] EN 993-19
PLC (1600 °C / 2912 °F) -0,51 [%] ISO 2478
Refractoriness under Load T0 1460 [°C] ISO 1893
Refractoriness under Load T0,5 1590 [°C] ISO 1893
- with load 0,200 [N/mm2]
Refractoriness under LoadT1 1600 [°C] ISO 1893
Refractoriness under LoadT2 1600 [°C] ISO 1893
Hot load test (25 psi) ASTM C16
- at test temperatures 2.640 [°F]
- schedules 3
- holding time 1,5 [h]
- change in length -0,06 [%]
Hot load test modified (175kPa/25 psi) ASTM C16
- at test temperatures 2.750 [°F]
- schedules 6
- holding time 1,5 [h]
- change in length -0,15 [%]
Res. to Thermal Shocks Water 30 [cycles] DIN 51068-1
Thermal Conductivity 400 °C / 752 °F 3,40 [W/mK] EN 821-2
800 °C / 1472 °F 2,90 [W/mK] EN 821-2
1000 °C / 1832 °F 2,75 [W/mK] EN 821-2
1200 °C / 2192 °F 2,70 [W/mK] EN 821-2
3
Abrasion 8,50 [cm ] ASTM C704
calibrated
CO-Resistance (class) A ASTM C288

The indicated values are standard values, i.e. values taken over a longer representative period of time according to either valid test
standards or internal test methods. They may not be regarded as committed specifications and therefore not as guaranteed
properties. We reserve the right to further technical developments and new editions of technical product information.

Revision: 01. MAY. 2022

RESISTAL A90-MX 2 / 2

Das könnte Ihnen auch gefallen